- 1.2210, DIN 115CrV3, AISI L2 round bar
- 1.2210, DIN 115CrV3, AISI L2 forging
- 1.2210, DIN 115CrV3, AISI L2 sheet
- 1.2210, DIN 115CrV3, AISI L2 flat bar
- 1.2210, DIN 115CrV3, AISI L2 pipe
1.2210, DIN 115CrV3, AISI L2
Production specification
Square-shape steel: 1mm to 4000mm
Plate steel:0.1mm to 4000mm
Width: 10mm to 2500mm
Lenth: We can supply any lenth based on the customer's requirement.
Forging: Shafts with flanks/pipes/tubes/slugs/donuts/cubes/other shapes
Tubings: OD: φ6-1800mm, with wall thickness ranging from 1-35 mm.
Finished goods condition: hot forging/hot rolling + annealing/normalizing + tempering/quenching + tempering/any conditions based on the customer's requirement
Surface conditions: scaled (hot working finish)/ground/rough machining/fine machining/based on the customer's requirement
Furnaces for metallurgical processing: electrode arc + LF/VD/VOD/ESR/Vacuum consumable electrode.
Ultrasonic inspection: 100% ultrasonic inspection for any inperfections or based on the customer's requirementExcellent service for all kinds of industries,with advantages of technologies, equipment and price.
We serve you with our honesty, integrity, and professionality.
1.2210, DIN 115CrV3, AISI L2
Designation by Standards
Brand Name | LH No. | Mat. No. | DIN | EN | AISI |
OCR1 | 804 | 1.2210 | 115CrV3 | - | L2 |
Chemical Composition (in weight %)
C | Si | Mn | Cr | Mo | Ni | V | W | Others |
1.17 | 0.23 | 0.30 | 0.65 | - | - | 0.10 | - | - |
Description
Low alloyed cold working steel/" target="_blank" class="keylink">tool steel.
Applications
Spiral and tap drills, broaching tools, engraving tools, ejectors, metal saws.
Physical properties (avarage values) at ambient temperature
Modulus of elasticity [103 x N/mm2]: 210
Density [g/cm3]: 7.80
Thermal conductivity [W/m.K]: 33.5, 32 (500oC), 31 (700oC)
Electric resistivity [Ohm mm2/m]: 0.33
Specific heat capacity[J/g.K]: 0.46
Coefficient of Linear Thermal Expansion 10-6 oC-1
20-100oC | 20-200oC | 20-300oC | 20-400oC | 20-500oC |
11.8 | 12.5 | 12.9 | 13.5 | 13.7 |
Soft Annealing
Heat to 710-850oC, cool slowly in furnace. This will produce a maximum Brinell hardness of 223.
Stress Relieving
Stress relieving to remove machining stresses should be carried out by heating to approx. 650oC, holding for 1-2 hours at heat, followed by air cooling. This operation is performed to reduce distortion during heat treatment.
Hardening
Harden from a temperature of 780-820oC, 800-840oC followed by water or oil quenching. Hardness after quenching is 64-66, 64-66 HRC.
Tempering
Tempering temperature: 100-400oC.
Tempering Temperature (oC) vs. Hardness (HRC)
100oC | 200oC | 300oC | 400oC | 450oC |
64 | 63 | 59 | 54 | 47 |
Tempering Diagram
Forging
Hot forming temperature: 1050-850oC.
Machinability
No data.
Corrosion Resistance
This is an steel/" target="_blank" class="keylink">alloy steel and it is not corrosion resistant. It will rust unless protected.
Mechanical properties
Heat treatment
Machining
Welding performance
Related hot word search:1.2210 DIN 115CrV3 AISI L2 round bar 1.2210, DIN 115CrV3, AISI L2,forging 1.2210, DIN 115CrV3, AISI L2,1.2210, DIN 115CrV3, AISI L2 sheet,coil 1.2210, DIN 115CrV3, AISI L2,1.2210, DIN 115CrV3, AISI L2 flat bar,pipe 1.2210, DIN 115CrV3, AISI L2,1.2210, DIN 115CrV3, AISI L2 Lrregular
Prev:1.1554, DIN C110W, AISI W1
Next:1.3505, DIN 100Cr6, AISI 5210